PV Module Abnormalities: Cell Chipping and Fragmentation
Release time:2025-07-23
Release time:2021-09-15
Author:
Author:
As photovoltaic (PV) module technologies continue to evolve toward higher efficiency and larger formats, quality control challenges in module manufacturing have become increasingly complex. Among the various production-related abnormalities that can lead to module performance degradation, corner chipping and microcracks at the busbar positions of solar cells are among the most frequently observed issues. These defects not only affect module appearance but may also compromise long-term electrical performance and reliability.Based on production-line observations and process analysis, the following factors are commonly associated with cell chipping or microcrack formation during PV module manufacturing.
Vertical Ribbon Edge Caused by Improper Flattening
During the tabbing or stringing process, the interconnecting ribbon between adjacent solar cells is flattened by a pressing mechanism. This step is intended to increase the contact area between the ribbon and the cell edge, thereby reducing localized mechanical stress.
However, if the flattening mechanism malfunctions or the ribbon feeding system operates abnormally, the ribbon may remain partially upright or stand on its edge. In such cases, the contact area between the ribbon and the cell edge is significantly reduced, resulting in excessive localized pressure. This condition can easily lead to microcracks or corner chipping at the solar cell edge.
Insufficient Cell Spacing
In TOPCon module production, the interconnecting ribbon electrically links the front side of one cell to the rear side of the adjacent cell, making cell spacing a critical process parameter. Even after flattening, ribbon thickness typically remains in the range of 0.1–0.15 mm.
If the spacing between neighboring cells is too narrow, the ribbon exerts excessive compressive force at the cell edge during subsequent processes. This increased pressure significantly raises the risk of microcracks or chipping, particularly at the busbar or edge regions.
Edge Sealing Defects
Abnormalities during the dual-glass module edge sealing process can also contribute to cell chipping or microcrack formation. If mechanical stress causes chipping prior to lamination, the resulting fragments are often found at a noticeable distance from the main cell body, providing a clear indication that the damage occurred before the lamination stage.

Glass Warping Induced by High Lamination Temperature
In cases where no abnormalities are observed at middle-hole positions after lamination, but chipping is present at cell edges near the ribbon, and other causes have been excluded, thermal effects during lamination should be considered.
A rapid temperature increase inside the laminator can cause the glass to warp or deform temporarily. This deformation may introduce localized mechanical stress at the ribbon-to-cell interface, leading to chipping around the affected positions.
Edge Sealing Defects Solder Balls or Slag on the Ribbon
During the stringing process, improper soldering conditions may result in solder balls or slag adhering to the ribbon surface. During lamination—particularly in the first vacuum chamber—the vacuum pressure or compressive force transmitted through the silicone membrane and glass can transfer localized stress through the ribbon to the cell.
If solder residues are present, this stress concentration can lead to cell edge chipping or fragmentation at the corresponding locations.
Conclusion
Throughout the PV module manufacturing process, both pre-lamination and post-lamination stages present multiple risk factors that can lead to solar cell chipping or microcrack formation. Effective control of ribbon flattening, cell spacing, soldering quality, edge sealing, and lamination temperature profiles is essential.
By strengthening process monitoring and implementing targeted inspections at each critical step, manufacturers can significantly reduce defect rates, improve module reliability, and ensure consistent high-quality production.