Abnormalities in Solar Plate Making Machine – EVA

Release time:2024-09-25

Release time:2021-09-15

Author:

Author:


During the operation of the solar module production line, certain abnormalities may occur with the materials used in solar panels. For experienced photovoltaic module manufacturers, taking preventative measures against such abnormalities can effectively reduce losses during the production process. Below is an analysis of the abnormalities related to the EVA used in photovoltaic modules.

 

Degree of Crosslinking

 

Definition of Crosslinking: It is a physical quantity used to characterize the degree of polymer crosslinking. The crosslinking degree of EVA can be represented by the gel content, which is the percentage of EVA gel (crosslinked EVA) in the EVA sample. The normal range of EVA crosslinking degree is 75%–95%, and the normal range of POE crosslinking degree is 65%–95%. The main methods currently used to measure the degree of crosslinking are:

 

1. Xylene extraction method

2. DSC (Differential Scanning Calorimetry)

 

Main Factors Affecting the Degree of Crosslinking: Lamination Time and Temperature

 

Generally, the crosslinking degree is positively correlated with lamination time and temperature. That is, when the temperature is constant, the longer the lamination time, the higher the degree of crosslinking. Similarly, when the lamination time is constant, the higher the lamination temperature, the higher the degree of crosslinking.

 

Note: The degree of crosslinking does not grow linearly; after reaching a certain level, the crosslinking rate will gradually slow down.

 

Methods for Adjustment and Troubleshooting:

 

1. Increase the lamination time

2. Increase the lamination temperature, focusing on the temperature of both chambers in a dual-chamber laminator

3. Measure the dynamic temperature of the laminator and check the uniformity of the heating plate temperature

4. Ensure uniformity in sample preparation (e.g., mesh bag standard, accuracy in weighing).

 

Bubbles on the Surface of the Solar Cells

Possible Causes of Abnormalities:

 

1. The laminator temperature is set too high, causing the crosslinking rate during the vacuum stage to be too fast, preventing some gases from being fully evacuated.

2. Abnormal vacuum in the laminator prevents maintaining a normal vacuum state.

3. Local gel deficiency, usually caused by uneven weight distribution of the encapsulation film.

4. Loose or damaged silicone sheets in the laminator.

5. Unreasonable lamination parameters.

 

Solutions:

1. Lower the lamination temperature, and to ensure sufficient crosslinking, slightly extend the lamination time.

2. Check the laminator seals, vacuum pump status, and the condition and lifespan of the silicone sheet.

3. Set reasonable lamination parameters based on the crosslinking curve, focusing on the relationship between temperature and vacuum time.

4. For new module designs, adjust the weight of the encapsulation film based on the thickness of the busbar.

 

Bubbles in Blank Areas, Busbar Bubbles, and Bubbles at Openings

(This type of bubble typically appears in dual-glass modules)

Possible Causes of Abnormalities:

1. The busbar is too thick, causing gel deficiency at the corners of the busbar due to insufficient encapsulation film.

2. Lack of proper tooling or improper tooling dimensions, leading to uneven pressure distribution on the module.

3. Abnormal vacuum or temperature (though this is less likely).

4. Instability in the encapsulation film itself.

 

Solutions:

1. Add small strips or blocks of encapsulation film at the corners of the busbar, with the number of layers adjusted based on the actual results (usually 1–2 layers).

2. Increase the weight of the encapsulation film.

3. Design appropriate lamination tooling for dual-glass modules.

4. If bubbles are present at openings in dual-glass modules, fill the space in the opening with small blocks of encapsulation film.

 

Edge Bubbles in Dual-Glass Modules

Possible Causes of Abnormalities:

1. Lack of proper tooling or improper tooling dimensions, leading to uneven pressure distribution on the module.

2. Mismatch in the selection of edge-sealing tape.

3. Insufficient weight of the encapsulation film.

 

During the lamination process, the edges of the module are subjected to greater force than the center. Dual-glass modules differ from conventional single-glass modules in that both sides of dual-glass modules are rigid glass structures, whereas the panel of a single-glass module is a flexible structure. During the lamination process, the heat stress on the edges is downward, and after lamination, there is reverse cooling stress. The rigid structure of dual-glass modules tends to lift outward when subjected to cooling stress, making them prone to reverse-suction bubbles.

 

Solutions:

1.Add small strips or blocks of encapsulation film at the corners of the module, with the number of layers adjusted based on the actual results (usually 1–2 layers).

2. Design appropriate lamination tooling or protective corners for dual-glass modules.

 

Delamination

Possible Causes of Abnormalities:

1. Contaminants between the encapsulation film and the glass or solar cells.

2. Insufficient weight of the encapsulation film.

3. Encapsulation film not fully melted.

 

Solutions:

1. Identify the source of contamination and eliminate the hazard.

2. Increase the weight of the encapsulation film.

3. Change the batch of encapsulation film.

 

Cell Breakage

Possible Causes of Abnormalities:

1. Insufficient weight of the encapsulation film.

2. Rapid inflation rate.

3. Excessive pressure on the module.

4. Excessive fluidity of the encapsulation film.

 

Solutions:

1. Increase the weight of the encapsulation film.

2. Ensure the lamination parameters are set within reasonable limits.

3. Reduce the fluidity of the encapsulation film.

 

About CHINTIYAN

Supplier of solar panel making machine,Photovoltaic module equipment manufacturing factory from China.

Customized solutions for solar panel production lines from 5MW to 1GW

Supply and delivery of nearly 30 types of equipment including Stringer Machines, Scribing Machines, IV Testers, and more

Optimization and upgrading of outdated solar panel production line capacity