Vacuum Bubbles (Snowflake-Pattern Bubbles) Inside PV Modules
Release time:2025-07-11
Release time:2021-09-15
Author:
Author:
During the PV module lamination process, vacuum bubbles—commonly referred to as snowflake-pattern bubbles—may occasionally appear inside the active area of the module rather than along the edges. This phenomenon not only affects the visual quality of the module but may also indicate underlying process control issues within the lamination stage. This article analyzes the formation mechanism of internal vacuum bubbles from both process and equipment perspectives, providing practical guidance for quality improvement.

Basic Mechanism of Snowflake-Pattern Bubble Formation
The formation mechanism of internal snowflake-pattern bubbles is fundamentally consistent with that of edge bubbles observed in frameless lamination processes. Both originate from localized pressure imbalance during lamination, which leads to temporary deformation of the front glass.
During lamination, the module stack is subjected to vacuum, heat, and mechanical pressure from the laminator's silicone membrane. Under normal conditions, pressure distribution across the heating plate and module surface should be uniform. However, when localized overpressure occurs, slight elastic deformation of the glass may take place.
This deformation typically remains within the elastic limit of the glass and is not immediately visible during lamination.

Role of Localized Overpressure
Localized overpressure is most commonly caused by foreign contaminants or uneven residues present on the surface of the laminator heating plate. Even small particles can create pressure concentration points when the silicone membrane presses the module stack against the heating plate.
Under such conditions:
- The front glass experiences minor downward deformation at the pressure concentration point.
- The distance between the front and back glass (or between glass and backsheet) is temporarily reduced in that localized area.
- EVA or POE encapsulant is compressed unevenly during the gelation stage.
Once the lamination cycle is completed, the silicone membrane releases pressure and the module is cooled. At this stage:
- The previously deformed front glass rebounds elastically to its original flat state.
- The local interlayer spacing increases suddenly in the rebound area.
Because the module interior has already been sealed under vacuum conditions, external air cannot re-enter to compensate for the increased internal volume.
As a result, a localized vacuum cavity forms within the encapsulant layer, manifesting visually as snowflake-pattern bubbles in the central area of the module.
Key Characteristics of Internal Snowflake Bubbles
- Occur inside the module, not at edges
- Typically appear after lamination or during cooling
- Often irregular or crystalline in shape
- Closely related to localized pressure anomalies rather than encapsulant material defects alone
Process Control Considerations
To reduce the occurrence of internal vacuum bubbles, attention should be given to the following aspects of lamination process control:
- Regular cleaning and inspection of laminator heating plates
- Ensuring flatness and cleanliness of silicone membranes
- Maintaining uniform pressure distribution during lamination
- Monitoring lamination pressure profiles and temperature uniformity
Effective control of these parameters helps ensure stable encapsulation quality and reduces the risk of internal bubble formation.
Conclusion
Vacuum-induced snowflake-pattern bubbles inside PV modules are primarily caused by localized pressure-induced glass deformation during lamination, followed by elastic rebound after pressure release. This phenomenon highlights the importance of equipment cleanliness, pressure uniformity, and precise lamination process control. Through systematic optimization of lamination conditions, the occurrence of such internal defects can be effectively minimized, contributing to improved module reliability and appearance quality.